PU gule Two component Polyether polyols for air filters
Instructions:
1. Material-A should stirred evenly with plastic hand electric drill, material-B can shake, before used.
2. Open the electrocaloric plate temperature to 40-50 degrees, in winter material-A and material-B with a small container to preheat.
3. Wipe the mould with release agent
4. According to the local environment, such as the humidity in the air, workshop environment.
5. material-A and material-B are mixed at the mixture ratio of 100:40 ratio, then add 40% talcum powder(heavy calcium powder)(100:40:50±5), with 2800 rev / min motor to mix, mixing time determined by the amount of adhesive, per 100g of adhesive is approximately 7-10 seconds .
6. Pour the Mixed liquid into mould, then put the paper element and give a little pressure on it. 8-15 minutes later you can bring the mould down